Home » Blog&News » 34CrNiMo6 (1.6582) vs AISI 4140 (42CrMo4): When Heavy Shafts Need Nickel

34CrNiMo6 (1.6582) vs AISI 4140 (42CrMo4): When Heavy Shafts Need Nickel

Author: Site Editor     Publish Time: 2026-10-08      Origin: Site

Inquire

facebook sharing button
twitter sharing button
line sharing button
wechat sharing button
linkedin sharing button
pinterest sharing button
whatsapp sharing button
sharethis sharing button

4140 and 34CrNiMo6 are both quenched-and-tempered engineering steels, and on a price list they sit one line apart. On a drawing they behave very differently once the section gets thick. 4140 (its European counterpart is 42CrMo4, 1.7225) is the volume workhorse of the alloy steel world — cheap, widely stocked, and perfectly adequate for shafts up to roughly 100 mm. 34CrNiMo6 (1.6582) takes the same Cr-Mo base and adds 1.30–1.70 % nickel, which is what allows a 400 mm rotor shaft to carry near-surface toughness all the way to the core. The procurement question is not which steel is "better" — it is at what diameter the nickel starts paying for itself.

Quick Comparison


AISI 4140 / 42CrMo4 (1.7225)

34CrNiMo6 (1.6582)

Standard

ASTM A29 / SAE J404; DIN EN 10083-3

DIN EN 10083-3

Alloy family

Cr-Mo

Ni-Cr-Mo

Nickel content

none (residual only)

1.30 – 1.70 %

Typical supply form

Hot rolled / forged bar, 6 – 250 mm

Forged bar and blocks, 50 – 800 mm

QT tensile (typical)

850 – 1300 MPa depending on section

900 – 1100 MPa

Character

High strength, moderate toughness

High strength with high toughness in large sections

Relative cost

Reference

~25 – 40 % higher (Ni surcharge)

Chemical Composition: One Element Changes the Grade

The table below lists the specification ranges. 4140 is shown in both its ASTM and DIN versions so you can see how close 4140 and 42CrMo4 really are — they are effectively interchangeable for most Q&T bar work.

Element (%)

AISI 4140 (ASTM A29 / SAE J404)

42CrMo4 (EN 10083-3)

34CrNiMo6 (EN 10083-3)

Carbon (C)

0.38 – 0.43

0.38 – 0.45

0.30 – 0.38

Manganese (Mn)

0.75 – 1.00

0.60 – 0.90

0.50 – 0.80

Silicon (Si)

0.15 – 0.35

≤ 0.40

≤ 0.40

Chromium (Cr)

0.80 – 1.10

0.90 – 1.20

1.30 – 1.70

Nickel (Ni)

—

—

1.30 – 1.70

Molybdenum (Mo)

0.15 – 0.25

0.15 – 0.30

0.15 – 0.30

Phosphorus (P), max

0.035

0.025

0.025

Sulfur (S), max

0.040

0.035

0.025

Three things stand out. First, 34CrNiMo6 carries less carbon than 4140 — 0.30 – 0.38 % against 0.38 – 0.43 %. That is deliberate: lower carbon means higher tempering resistance is not needed to hit the strength, but weldability and impact energy both improve. Second, the chromium climbs from roughly 1 % to 1.5 %, deepening hardenability on its own. Third — the headline change — 1.30 – 1.70 % nickel. Nickel does almost nothing for hardness; what it does is lower the ductile-to-brittle transition temperature and multiply toughness at a given strength level.

What Nickel Actually Buys You

Hardenability in real sections. A Cr-Mo steel like 4140 hardens well in a 50 mm bar oil-quenched from 840 – 860 °C. Past about 100 mm, the cooling rate at the core is too slow for the available hardenability: the core transforms to mixed microstructure, and the hardness gap between surface and center grows. Nickel is the most powerful conventional austenite stabilizer for delaying that transformation, and combined with the higher chromium in 34CrNiMo6, the grade holds a usable Q&T core in sections beyond what 4140 can reach. This is why gear and rotor forgings in the 200 – 600 mm range are specified in 34CrNiMo6 or its bigger sibling 30CrNiMo8 (1.6580), not 4140 — see the 30CrNiMo8 product page for its chemistry.

Toughness at strength. At a matched tensile strength of 900 – 1000 MPa, 34CrNiMo6 typically delivers impact energy around 40 J or better at room temperature, and keeps useful toughness at −20 °C and below. 4140 at the same strength is more notch-sensitive — acceptable for many machine shafts, a liability for rotating equipment that sees impact, low temperature, or where a fracture would be catastrophic.

Distortion and tempering control. The lower carbon of 34CrNiMo6 gives a wider, safer tempering window and less quench-crack risk on sharp-featured forgings. 4140 at 0.43 % C needs a more disciplined quench-and-temper practice, especially on complex sections.

Mechanical Properties: Matched Strength, Different Sections

Typical quenched-and-tempered values as published on our product pages; final figures always come from the EN 10204 3.1 certificate of the actual heat.

AISI 4140 / 42CrMo4 — Q&T, by section size:

Diameter

Yield Rp0.2 (min)

Tensile Rm

Elongation A (min)

Impact KV (RT)

Hardness

≤ 16 mm

900 MPa

1100 – 1300 MPa

10 %

≥ 30 J

32 – 38 HRC

16 – 40 mm

750 MPa

1000 – 1200 MPa

11 %

≥ 35 J

30 – 36 HRC

40 – 100 mm

650 MPa

900 – 1100 MPa

12 %

≥ 40 J

28 – 34 HRC

100 – 160 mm

600 MPa

850 – 1000 MPa

13 %

≥ 45 J

26 – 32 HRC

160 – 250 mm

550 MPa

800 – 950 MPa

13 %

≥ 45 J

24 – 30 HRC

34CrNiMo6 — Q&T, typical:

Property

QT (typical)

Tensile strength Rm

900 – 1100 MPa

Yield strength Re

≥ 700 MPa

Elongation A5

≥ 12 %

Impact KV at 20 °C

≥ 40 J

Hardness

248 – 341 HB

Read the two tables together and the pattern is clear: at 40 – 100 mm both steels land in a similar strength band, and 4140 wins on price. The divergence happens above that — 4140's achievable core properties slide down the diameter bands, while 34CrNiMo6 holds its numbers into sections several times larger.

Heat Treatment Practice

4140 is austenitised at 840 – 860 °C, oil-quenched and tempered in the 540 – 680 °C range depending on the target hardness. 34CrNiMo6 is oil-quenched from 850 – 880 °C and tempered between 580 – 660 °C. On large forgings the tempering cycle is tuned to the actual section — for diameters above 600 mm the hold times and ramp rates matter as much as the temperatures, and hardness mapping across the section is the only honest way to verify through-hardening. Both grades should be tempered well away from the 250 – 400 °C embrittlement range, and 34CrNiMo6's nickel content gives extra insurance against temper embrittlement on slow-cooled heavy sections.

Typical Applications Side by Side

4140 / 42CrMo4: machine shafts and spindles up to ~100 mm, gears and pinions, bolts and studs (class 10.9 / 12.9), injection mold bases, general machinery parts. It is also the starting point for nitriding work — see our AISI 4140 product page for supply conditions.

34CrNiMo6: power generation rotor shafts and turbine discs, marine propeller shafts and rudder stocks, large gear and pinion shafts, mill rolls, oil & gas drilling subs — anywhere the section is large, the stress is high, and a brittle failure is unacceptable. Full capability details are on our 34CrNiMo6 (1.6582) product page.

Selection Guide

  1. Section ≤ 100 mm, general machine duty → 4140. No reason to pay the nickel surcharge.

  2. Section 100 – 250 mm, moderate duty → evaluate case by case. 4140 can still work if the core requirement is modest; otherwise step up.

  3. Section > 250 mm, rotating or impact duty, sub-zero service → 34CrNiMo6 (or 30CrNiMo8 for the heaviest rotors).

  4. Drawing calls out ASTM 4340 → note that 4340 (0.38 – 0.43 % C, 1.65 – 2.00 % Ni) is closer to 34CrNiMo6 than to 4140 in behavior; our 4140 vs 4340 comparison covers the differences in detail.

Frequently Asked Questions

Is 34CrNiMo6 the same as 4340?

No. The closest US counterpart of 34CrNiMo6 is the 4337 family; 4340 carries more carbon (0.38 – 0.43 %) and more nickel (1.65 – 2.00 %), which pushes strength higher but reduces weldability further. For new tooling that calls up an ASTM grade, send us the spec and we will confirm the closest supply option and any heat-treatment adjustment.

Can 4140 be through-hardened at 300 mm diameter?

Not in any meaningful sense. The core cooling rate at that section is far below what 4140's hardenability needs; you will get a hard case and a substantially softer core. If the application depends on core properties, specify 34CrNiMo6 or 30CrNiMo8 and verify with hardness mapping.

Which grade should I use for −40 °C service?

34CrNiMo6. Nickel lowers the ductile-to-brittle transition temperature, which is precisely the property 4140 lacks. For low-temperature rotating equipment, ask for impact testing at the service temperature on the certificate.

What certificates come with the bars?

EN 10204 3.1 is standard on every shipment; 3.2 with third-party witness (ABS, BV, CCS, GL) is available on request.

Request a Quote

Send us the diameter, length, quantity, required condition and destination port — for either grade. You will get a technical proposal and quotation within 24 hours.

Email: enquiry@qilumetal.com | Web: www.qilumetal.com

SPECIALIZING IN SPECIAL STEEL SMELTING AND FORGING

About Us

Hunan Qilu Metal is one of the professional steel manufacturers and exporters in China, with multiple certificates such as ISO9001. Our products can be produced according to customer requirements, with a small minimum order quantity and affordable prices.

Quick Links

Product Category

Contact Us

Tel:+86-731-85185765
Email:enquiry@qilumetal.com
Address:Room 2832, Building B3 to B6, Taskin Urban Plaza, No. 18 Xiangfu Middle Road,Yuhua District, Changsha City
Copyright 2023 © Hunan Qilu Metal Co.,Ltd.  All rights reserved.  Support by Leadong|Sitemap|Privacy Policy